AsphaltTons.com — asphalt tonnage calculator

Asphalt Draindown Test: How AASHTO T 305 Works

The asphalt draindown test answers one plain question: if this mix sits hot in a silo or a truck bed, will the binder stay on the stone or slowly run off it? It matters most for stone matrix asphalt (SMA) and open-graded friction course (OGFC). Both mixes carry a lot of binder on a coarse stone skeleton with very little fine material to hold it in place. This guide covers how the test is run under AASHTO T 305, what the numbers mean, the limits state DOTs use, and what a plant does when a sample fails.

Converting a mix design to tons for a job? Open the asphalt tonnage calculator →

What "draindown" actually means

AASHTO T 305 defines draindown material as whatever separates from the sample and ends up outside the wire basket during the test. That can be asphalt binder alone, or binder carrying fine aggregate with it. On a job you see the same thing as a puddle of binder in the truck bed, or as fat, shiny spots in the finished mat where rich mastic collected.

Dense-graded mixes rarely have this problem, because their fine particles act like a sponge for the binder film. The FHWA's OGFC how-to document puts it simply: open-graded mixes typically have little material passing the No. 4 (4.75 mm) sieve and a relatively low amount passing the No. 200 sieve, so there is not much to hold a thick binder film in place. SMA has the same issue for a slightly different reason. It is built on stone-on-stone contact with a rich mastic, and its specs call for a high binder content. New York's SMA spec, for example, sets a 6.5% minimum.

The equipment

The test needs very little gear, which is part of why plants can run it every day:

  • Standard wire basket. Made from 6.3 mm (1/4 in) sieve cloth, 165 mm deep and 108 mm wide, with the basket floor raised 25 mm above the bottom of the assembly, per the INDOT and MoDOT versions of the method. The raised floor lets drained material fall clear instead of wicking back up.
  • A plate or pan under the basket. T 305 says cake pans or pie tins work, and several DOT versions use paper plates. A reusable option is a heavy aluminum tin like these KitchenDance 9 in heavy-duty aluminum pie tins. Weigh each one empty, every time, because the test result is the change in its weight.
  • Forced-draft oven that holds a setting between 250 and 350°F within ±3.6°F (±2°C). A cheap dial gauge such as the Rubbermaid stainless oven monitoring thermometer (60–580°F) is handy for a quick check that a shop oven isn't drifting, but it is not a calibration device. Use the lab's calibrated thermometer for the record.
  • Balance readable to 0.1 g. With samples near 1,200 g, you need room for the basket too. Bench scales like the U.S. Solid 5,000 g × 0.1 g precision balance read to 0.1 g, but the maker lists accuracy as ±0.2 g. Check that against the balance requirement your agency's method references before relying on it for acceptance.

How the test is run, step by step

This follows the INDOT summary of T 305 and Missouri's TM-61, which is MoDOT's adaptation of the original NCAT procedure:

  1. Get the sample. Lab samples are mixed to the job mix formula. MoDOT uses 1,200 g, with any fiber stirred into the dry aggregate before the binder goes in. Plant samples come from trucks before they leave the plant and are quartered down to test size. South Carolina's SC-T-90 targets 1,000 to 1,500 g.
  2. Load the basket loosely. Put the whole sample into the tared basket and don't tamp, press or shake it. Weigh the sample to 0.1 g.
  3. Weigh the plate to 0.1 g, set the basket on it, and note the mix temperature.
  4. Heat for one hour at the plant production temperature (INDOT allows 60 ± 5 minutes). If the sample has cooled more than 77°F below the test temperature before going in, INDOT runs it 70 ± 5 minutes instead.
  5. Weigh the plate again. Lift the basket away and weigh only the plate with whatever dripped onto it. MoDOT notes that any obvious stone particles that fell through should go back into the mix rather than be counted, or the test should be rerun.
  6. Run duplicates. The reported result is the average of two tests.

During mix design, many agencies also test at a temperature above production. That shows what happens on a day when the burner runs hot. New York and New Jersey SMA specs call for production temperature and 15°F higher, and the FHWA OGFC document cites research recommending 27°F above the expected production temperature.

The calculation, with a worked example

The math is one line:

Draindown, % = (final plate mass − initial plate mass) ÷ initial sample mass × 100

INDOT's own example uses a plate that went from 1,285.6 g to 1,289.3 g under a 1,150.8 g sample. That is 3.7 g of drained material, or 0.32%, which would fail a 0.30% maximum. Here is a second, made-up pair of duplicates to show how the average works:

Sample mass (C)Plate before (B)Plate after (A)A − BDraindown
INDOT example1,150.8 g1,285.6 g1,289.3 g3.7 g0.32% (fails 0.30)
Duplicate 1 (illustrative)1,204.6 g152.4 g154.1 g1.7 g0.14%
Duplicate 2 (illustrative)1,198.2 g151.9 g153.9 g2.0 g0.17%
Reported result for the pair0.15%

Notice how small the numbers are. The difference between passing and failing in the INDOT example is well under half a gram on a sample the size of a brick. That's why a 0.1 g balance, a consistent pan, and leaving the sample undisturbed matter so much.

To put the limit in tons: 0.3% of a ton of mix is 6 lb (2,000 × 0.003). On a 20-ton load that would be about 120 lb of binder and fines. That's just arithmetic for scale; a truck is not a lab basket.

Draindown limits in real specifications

Most agencies land on the same number, but how they test and what they do about a failure varies. Figures below were checked against each agency's published document in November 2026.

Agency and mixDraindown limitNotable detail
New York State DOT, SMA (built on AASHTO M 325)0.30% max (T 305)Each lot is tested at production temperature and 15°F above. If it fails, production stops until corrections are approved.
Ohio DOT Item 443, SMA0.3%Draindown test once per production day. If the limit is exceeded, fiber dosage goes up 0.1%. The spec also caps storage at 2 hours and mix temperature at 350°F.
Minnesota DOT, SMAUnder 0.3% (1-hour reading)One test per 500 tons. On a failure, check that the stabilizer is actually being added, that the rate is right, and that mixing temperature isn't excessive.
New Jersey DOT, SMA0.30% maxProduction tests are run at 15°F above the mixing temperature.
Georgia DOT, 9.5 and 12.5 mm OGFC and 12.5 mm PEMUnder 0.3% (T 305)Fiber is required in all OGFC and PEM. A fiber product must hold draindown to 0.2% or less in a standard mix to be approved.
South Carolina DOT, OGFC (SC-T-90)Under 0.5% (99.5% minimum retention)Reports binder retained as a share of the binder in the sample rather than of the whole mix, with the oven at 350 ± 5°F.

The South Carolina line is a reminder to read the method your agency names. A percent of binder and a percent of total mix are different denominators. A mix at about 6% binder that loses 0.3% of its binder has lost far less than 0.3% of the mix.

What fixes a failing draindown result

Plants generally have four levers, and the specs above name most of them:

  • Fiber dosage. Cellulose or mineral fiber gives the binder something to cling to. Georgia's fiber spec lists cellulose at 0.2–0.4% and mineral fiber at 0.3–0.6% of total mix. In tonnage terms, 0.3% cellulose is about 6 lb of fiber per ton, and Ohio's 0.1% bump adds about 2 lb per ton.
  • Make sure the fiber is actually getting in. Minnesota's first check on a failure is whether the stabilizer is being added at all. A plugged or empty fiber feeder looks exactly like a bad mix design.
  • Temperature. Hotter binder is thinner. Minnesota tells contractors to check for excessive mixing temperature, and Ohio caps SMA at 350°F. A Georgia DOT research report notes that conventional OGFC once had to be placed at only 230–250°F because of draindown. Modified OGFC with polymer and fiber can be produced at roughly 320–338°F.
  • Binder and additives. The FHWA document lists cellulose, mineral fiber, crumb rubber, polymers and warm mix additives as stabilizers. South Carolina uses a warm mix additive instead of fibers in OGFC. Two NCAT test track sections built in 2012 with ground-tire-rubber binder and no fibers met draindown requirements during construction.
  • Storage time. Ohio's spec says that if draindown shows up, shorten the storage time and increase the fiber.

How it fits with the other mix tests

Draindown is a loose-mix test. It says nothing about strength or durability once the mat is compacted. With open-graded mixes it is usually balanced against the Cantabro abrasion test: more binder lowers raveling loss but raises draindown risk. For SMA it sits next to the volumetric checks covered in our stone mastic asphalt guide, and for plant-produced samples the binder content behind the numbers usually comes from the ignition oven. For background on why these mixes are built so open, see open-graded friction course explained.

Asphalt draindown test FAQ

What is the draindown test for asphalt?

It measures how much binder, or binder plus fines, runs off a loose sample of hot mix. Under AASHTO T 305 the sample sits in a 1/4 in mesh wire basket over a weighed plate for one hour at plant production temperature, and whatever lands on the plate is the draindown.

What is the maximum allowable draindown?

For stone matrix asphalt and open-graded friction course, most specs cap it at 0.3% of the total mix. New York, New Jersey, Ohio, Minnesota and Georgia all use 0.3%. South Carolina states its OGFC limit as a minimum 99.5% binder retention instead.

How do you calculate percent draindown?

Subtract the empty plate weight from the plate weight after the hour in the oven, divide by the starting sample weight, and multiply by 100. INDOT's example: 3.7 g drained from a 1,150.8 g sample is 0.32%. Report the average of two samples.

Why is draindown a problem for SMA and open-graded mixes?

Both are coarse mixes (SMA is gap-graded, OGFC open-graded) with little fine material to hold a thick binder film, and SMA also carries a high binder content (New York requires at least 6.5%). Without fiber or a stiffer binder, the film can drain during storage and hauling and leave fat spots in the mat.

How do plants fix a failing draindown result?

They check that the fiber feeder is actually adding fiber, raise the fiber dose (Ohio adds 0.1% after a failure), lower the mix temperature, and shorten storage time. Polymer, crumb-rubber or warm mix additives can also stabilize the binder.

The bottom line

The draindown test is a one-hour, one-basket check that the binder in an SMA or open-graded mix will stay where it belongs while the mix is stored and hauled. Weigh the pan before and after, divide by the sample mass, and average two runs. Most agencies cap the result at 0.3% of the mix. When a sample fails, the usual suspects are a fiber feeder problem, too much heat, or mix sitting too long. Pavements made from these mixes still get ordered and hauled by the ton, so when you're ready to price one, run your dimensions through the asphalt calculator.

Sources

As an Amazon Associate, AsphaltTons.com earns from qualifying purchases. Product links below are sponsored.