PG 58-28 Asphalt Binder: What It Means and Where It's Used
PG 58-28 is a performance grade for the asphalt binder (asphalt cement) that holds a hot mix together. The 58 and the minus 28 are pavement temperatures in Celsius: the binder is graded to resist rutting up to a hot-weather pavement temperature of 58°C (about 136°F) and to resist cold cracking down to a pavement temperature of −28°C (about −18°F). It is a cold-climate grade. You will see it all over specs and plant tickets in Michigan, Minnesota, Indiana and other northern states. Below: what the lab tests to earn the label, where agencies use it, and how the S, H, V and E letters fit in.
Pricing a job that calls for PG 58-28 mix? Open the asphalt tonnage calculator →Reading the two numbers
In the Superpave system, the first number is the average seven-day maximum pavement temperature the binder is meant for. The second is the minimum pavement design temperature. FHWA's Superpave guidance figures both at a depth of 20 mm (about 3/4 in) below the surface, and converts weather station air temperatures into pavement temperatures using models from the Long-Term Pavement Performance (LTPP) program.
Grades step in 6°C increments. A 58 sits between 52 and 64 on the hot end, and a −28 sits between −22 and −34 on the cold end. The design temperatures usually come with a reliability level. FHWA describes 98% reliability as two standard deviations past the average temperature, so a 98% grade covers a hot or cold year, not only a typical one.
Neither number is a thickness, a mix size or a brand. Our explainer on the low-temperature number covers the minus side in more detail.
What the lab tests to certify PG 58-28
Every PG grade is run through the same set of tests. The grade only sets the temperatures they are run at and a couple of pass/fail limits. The table below lists the AASHTO M 320 requirements for PG 58-28, checked against the Asphalt Institute's state binder spec sheet for Alaska (which lists PG 58-28 under M 320) and a PG 58-28 product data sheet from the refiner Moeve.
| Binder condition | Test (AASHTO) | Test temperature | Requirement |
|---|---|---|---|
| Original | Flash point (T 48) | n/a | 230°C (446°F) min. |
| Original | Rotational viscosity (T 316) | 135°C (275°F) | 3.00 Pa·s max. |
| Original | Dynamic shear, G*/sin δ (T 315) | 58°C | 1.00 kPa min. |
| After RTFO (short-term aging) | Mass change (T 240) | n/a | 1.00% max. |
| After RTFO | Dynamic shear, G*/sin δ (T 315) | 58°C | 2.20 kPa min. |
| After PAV (100°C, 20 hr, 300 psi) | Dynamic shear, G*·sin δ (T 315) | 19°C (66°F) | 5,000 kPa max. |
| After PAV | BBR creep stiffness (T 313) | −18°C (0°F) | 300 MPa max. |
| After PAV | BBR m-value (T 313) | −18°C | 0.300 min. |
A few things in that table trip people up:
- The high-temperature tests run at exactly 58°C. The binder must be stiff enough there both fresh and after the rolling thin-film oven (RTFO) simulates plant aging. This is the rutting check, run on a dynamic shear rheometer.
- The cold test runs at −18°C, not −28°C. Pavement Interactive's bending beam rheometer (BBR) reference explains why. For most binders, raising the test temperature by 10°C lets a 60-second load stand in for two hours of loading at the actual low design temperature. So every "−28" binder is beamed at −18°C. Our bending beam rheometer guide walks through the beam test itself.
- The intermediate test is a fatigue check. After pressure-aging vessel (PAV) aging, which mimics years in service, the binder can't be too stiff at 19°C. Michigan's binder special provision and Indiana's spec both allow up to 6,000 kPa when the phase angle is at least 42°.
Where agencies actually use PG 58-28
Michigan is a good example, because the grade shows up all over its design guidance. In MDOT's Road Design Manual binder table (section 6.03.09A1d, issued August 2026):
- In the Metro, North, Grand, Bay, Southwest and University regions, PG 58-28 is the top and leveling course binder for EL (lowest traffic) Superpave mixes. Base courses there get PG 58-22, except in the North Region, which uses PG 58-28.
- In the Superior Region (the Upper Peninsula), the top and leveling courses step down to PG 58-34 and PG 58-28 moves into the base course.
- Shoulders 8 ft or wider, or paved in a separate operation, get PG 58-28 top and leveling courses statewide.
- Temporary roads, commercial and private approaches, wedging and hand patching get PG 64-22 in most regions but PG 58-28 in the Superior and North regions.
MDOT's Local Agency Program HMA selection guidelines (updated January 27, 2026) carry this down to county and city roads. Outside the Superior Region, PG 58-28 is recommended for a commercial ADT of 0 to 300, and roads from 301 to 3,400 move up to PG 64-28. The same guide uses PG 58-28 for nearly every non-motorized path mix.
Minnesota uses an MSCR version of the grade, PG 58S-28. MnDOT's binder guidelines specify it for overlay wearing courses under 10 million ESALs and for everything more than 4 in below the surface. Indiana's spec sheet says INDOT has specified PG 58-28 binders under AASHTO M 332 since its September 2024 letting.
PG 58S-28, 58H-28, 58V-28 and 58E-28
States that adopted AASHTO M 332 keep the 58 and the −28 but add a letter for traffic: S for standard, H for heavy, V for very heavy and E for extremely heavy. The letter is checked with the multiple stress creep recovery (MSCR) test at 58°C on RTFO-aged binder, instead of bumping the high-temperature number. MnDOT's limits:
| Grade | Jnr at 3.2 kPa, max. (kPa⁻¹) | % recovery at 3.2 kPa, min. | MnDOT lets it replace |
|---|---|---|---|
| PG 58S-28 | 4.5 | Not required | PG 58-28 |
| PG 58H-28 | 2.0 | 30 | PG 64-28 |
| PG 58V-28 | 1.0 | 55 | PG 70-28 |
| PG 58E-28 | 0.5 | 75 | n/a |
So a Minnesota PG 58H-28 fills the role an older PG 64-28 spec did, and two documents can name the same binder in different ways.
How PG 58-28 compares with nearby grades
One quick way to compare grades is the spread between the two numbers. Pavement Interactive gives a rule of thumb: binders whose high and low grades differ by 90°C or more generally need some kind of modification, such as a polymer.
| Grade | High / low pavement temp | Spread | Typical role in Michigan guidance |
|---|---|---|---|
| PG 58-22 | 58°C / −22°C | 80°C | Base course in most MDOT regions |
| PG 58-28 | 58°C / −28°C | 86°C | Low-traffic top and leveling course, North Region base, UP base |
| PG 64-22 | 64°C / −22°C | 86°C | Approaches and hand patching in southern regions |
| PG 64-28 | 64°C / −28°C | 92°C | Medium-traffic (EML) top and leveling course |
| PG 58-34 | 58°C / −34°C | 92°C | Upper Peninsula top and leveling course |
PG 58-28 and PG 64-22 have the same 86°C spread. One trades 6°C of summer stiffness for 6°C more winter crack resistance, so the choice is mostly about climate. The 90°C rule is only a rule of thumb, though. MDOT's table marks polymer-modified grades with a "P" (PG 70-28P, PG 64-34P), but its plain PG 64-28 carries no P even with a 92°C spread.
When the grade gets "bumped"
FHWA's Superpave Mixture Design Guide suggests considering a higher high-temperature grade above 10 million ESALs and requires one grade higher above 30 million. It also recommends going up one grade for slow-moving traffic (20 to 70 km/h) and two grades for standing traffic (under 20 km/h). Bump for volume or for speed, not both.
Michigan handles this with a "High Stress" pay item for about 1,000 ft either side of signalized intersections, roundabouts and other stop-and-go spots. Where a road would otherwise get PG 58-28, MDOT's table lists PG 64-28 for EL High Stress mixes.
Worked example: reading a PG 58-28 test report
Here is a made-up daily binder sample from a Michigan project that specifies PG 58-28. The test results are illustrative. The limits and price reductions come from MDOT special provision 26SP-501C-03 and the M 320 limits above.
| Test | Result | Limit | Outcome |
|---|---|---|---|
| Original DSR at 58°C | 1.31 kPa | ≥ 1.00 kPa | Pass |
| RTFO mass change | 0.42% | ≤ 1.00% | Pass |
| RTFO DSR at 58°C | 2.05 kPa | ≥ 2.20 kPa | Out of spec, falls in the 1.98–<2.08 band: 5% reduction |
| PAV DSR at 19°C | 5,420 kPa, phase angle 43° | ≤ 6,000 kPa when phase angle ≥ 42° | Pass |
| BBR stiffness at −18°C | 286 MPa | ≤ 300 MPa | Pass |
| BBR m-value at −18°C | 0.297 | ≥ 0.300 | Out of spec, falls in the 0.292–<0.300 band: 2.5% reduction |
Two tests miss. Under MDOT's provision, when more than one test on a sample is out of spec, only the greatest single reduction applies. That makes it a 5% cut to the contract base price of the HMA mixture for the day of production the sample represents, not 7.5%. The same provision lets a contractor swap in a "better" grade at no extra cost. For a PG 58-22 base, PG 58-28 or PG 64-28 would qualify, and the binder is then tested against the grade actually used.
What this means for a driveway or parking lot
For a driveway you buy whatever surface mix the local plant is running, and in much of Michigan the low-traffic mixes are built around PG 58-28. A few practical points:
- Ask for the grade on the quote and look for it on the ticket. If one plant quotes PG 58-28 and another quotes PG 64-22, they're selling binders tuned for different climates, not two prices for the same thing.
- Grade doesn't change tonnage. At our 145 lb/ft³ planning density, a 12 ft × 50 ft driveway at 2 in compacted is 100 ft³, or 14,500 lb, which is about 7.3 tons, whatever the binder grade. Measure the area with a wheel like this Zozen collapsible measuring wheel and run the numbers through the asphalt calculator.
- Temperature still rules on paving day. MnDOT tells contractors to follow the binder supplier's mixing and compaction temperatures. As one example, Moeve's PG 58-28 data sheet lists 150–160°C (302–320°F) for mixing and 145–155°C (293–311°F) for compaction. Check the mix as it comes off the truck with an infrared gun like the Etekcity infrared thermometer (−58 to 1,130°F). Keep in mind it reads only the surface.
- Handwork matters more than grade at the edges. Seams and edges still need to be luted and rolled while hot. A magnesium lute such as the Kraft Tool 36 in asphalt lute head makes that easier.
Frequently asked questions
What does PG 58-28 mean?
PG stands for performance grade. The binder is graded for an average seven-day maximum pavement temperature of 58°C (about 136°F) and a minimum pavement design temperature of -28°C (about -18°F). Both are pavement temperatures near the surface, not air temperatures.
Is PG 58-28 a polymer-modified binder?
Usually not. Its high and low grades are 86°C apart, under the 90°C spread at which Pavement Interactive says binders generally need modification. Michigan DOT marks polymer grades with a P (for example PG 70-28P), and its PG 58-28 carries no P.
What is the difference between PG 58-28 and PG 64-22?
PG 64-22 is stiffer in summer heat (graded to 64°C instead of 58°C) but only graded down to -22°C. PG 58-28 gives up that 6°C of rutting resistance for 6°C more cold-cracking resistance, which is why northern states lean on it.
What is PG 58S-28?
It is PG 58-28 graded under AASHTO M 332, which adds the multiple stress creep recovery test. The S means standard traffic, with a Jnr of no more than 4.5 per kPa at 58°C. MnDOT accepts PG 58S-28 as a substitute for PG 58-28, and allows 58H-28 and 58V-28 as substitutes for the older PG 64-28 and PG 70-28.
Why is the bending beam test for PG 58-28 run at -18°C?
Testing 10°C warmer lets a 60-second beam load stand in for about two hours of loading at the -28°C design temperature, per Pavement Interactive. The beam must show creep stiffness of no more than 300 MPa and an m-value of at least 0.300.
The short version
PG 58-28 is a binder graded for pavements that reach about 58°C in a hot week and −28°C on the coldest night, proven with shear tests at 58°C, a fatigue check at 19°C and a beam test at −18°C. Northern DOTs use it for low-traffic surfaces, bases, shoulders and paths. On a quote it tells you the climate the binder was built for, not how many tons you need.
Sources checked November 18, 2026: MDOT Road Design Manual 6.03.09A1d asphalt binder selection (August 2026 update); MDOT Local Agency Program Hot Mix Asphalt Selection Guidelines (01/27/26); MDOT special provision 26SP-501C-03, price adjustments on PG asphalt binders; Asphalt Institute state binder spec sheets for Alaska (AASHTO M 320), Minnesota and Indiana (AASHTO M 332); MnDOT PG Binder Guidelines (MSCR) and Standard Specification 3151; FHWA Superpave Mixture Design Guide (FHWA-RD-01-052) and FHWA Level I mixture design notes; FHWA LTPPBind Online; Pavement Interactive, Superpave Performance Grading and Bending Beam Rheometer; Moeve PG 58-28 product data sheet.